Ink

HY Series Organic Bentonite Use Method

HY series organic bentonite is made by excellent bentonite with the processing of highly purified, modified and ion exchange into organic covering agent, it is a sheet structure product, if you want the organic bentonite to play a better performance, you need to separate its sheet-structure as much as possible. This process usually needs to be provided with mechanical energy, chemical energy and heat energy.

Use Method:

Dry powder method:

Dry powder method is that add the dry powder directly into the system during the production process, it doesn't need the polar activator, such as HY-2, HY-S2, HY-S3, HY-S34.

Pre gel method:

For poor wettability resin systems (such as epoxy, polyester, short oil alkyd resin etc. )it is better to use HY series organic bentonite by pre gel. 

(1) composed of pre gel: solvent 87%, organic bentonite 8-10%, polar activator 3-4%.

(2) preparation of pre gel: solvent and organic bentonite (mixed 10min, fully wettability), then add the polar activator (stirring for 5min, full expansion). 

Other information:

The dispersion speed

No matter you use any one method, bentonite products must be thoroughly dispersed to be a gel, so it can show its properties as thixotropy, anti settling and thickening effect, this kind of dispersion need extra high shear force, for example, to use high speed dispersion machine, three roller mill, colloid mill, sand grinding or milling. If the shear force and activation energy is enough, it is easy to obtain gel. The organic bentonite efficiency increased with the increase of dispersion speed.

Dispersion temperature

Increasing the temperature can also improve the gel property. The gel property with high temperature solvent is better than the low temperature (0 °C -5 °C ) solvent when the other conditions keep the same. But the dispersion temperature can not exceed the boiling point of activation solvent.

Activating agent

The polar additive can help the sheet-layer structure bentonite easily form a layer-sheet structure, thus formed a thixotropic gel, polar additives such as ethanol, methanol, acetone, propylene carbonate, the add amount of polar additives is generally 30%-50% of the organic bentonite.

Moisture

Organic bentonite must have enough moisture to develop into a network structure pre gel, the water molecules forming a bridge for the network structure, so the organic bentonite should not be too dry, the general moisture content should be around 3.5%, polar additives should not use anhydrous, the suitable content of the polar additives is appropriate 95% (the moisture is 5%).


主站蜘蛛池模板: 成年无码动漫av片在线尤物网站| 中文字幕在线不卡精品视频99| 国产毛片一区二区精品| 久久亚洲色www成人网址| 少妇被多人c夜夜爽爽av| 久久综合网丁香五月| 亚洲大尺度专区无码浪潮av | 人妻精品动漫h无码网站| 少妇高潮惨叫久久久久电影| 国内老熟妇乱子伦视频| 少妇人妻综合久久中文| 久久这里只精品国产免费9| 欧美做受视频播放| 成人国产精品日本在线观看| 无码中文av波多野结衣一区| 免费毛片a线观看| 内射人妻无套中出无码| 国产久爱免费精品视频| 久拍国产在线观看| 国产精品主播一区二区三区| 亚洲va中文字幕无码一二三区| 国产精品ⅴ无码大片在线看 | 亚洲日本高清一区二区三区| 久久一本人碰碰人碰| 极品少妇伦理一区二区| 国精品人妻无码一区二区三区d3| 欧美国产日韩亚洲中文| 免费无码作爱视频| 无套内射在线观看theporn| 亚洲人成绝费网站色www吃脚| 成人做爰www网站视频下载| 99国产精品欧美一区二区三区| 亚洲大成色www永久网站注册| 上海少妇高潮狂叫喷水了| 青青草在久久免费久久免费| 四虎成人永久在线精品免费| 人与动人物xxxx毛片人与狍| 免费观看性行为视频的网站 | 精品高潮呻吟99av无码视频| 亚洲国产成人高清影视| 亚洲精品屋v一区二区|